Abstract

In this research, multiexpression programming (MEP) has been employed to model the compressive strength, splitting tensile strength, and flexural strength of waste sugarcane bagasse ash (SCBA) concrete. Particle swarm optimization (PSO) algorithm was used to fine-tune the hyperparameter of the proposed MEP. The formulation of SCBA concrete was correlated with five input parameters. To train and test the proposed model, a large number of data were collected from the published literature. Afterward, waste SCBA was collected, processed, and characterized for partial replacement of cement in concrete. Concrete specimens with varying proportion of SCBA were prepared in the laboratory, and results were used for model validation. The performance of the developed models was then evaluated by statistical criteria and error assessment tests. The result shows that the performance of MEP with PSO algorithm significantly enhanced its accuracy. The essential input variables affecting the output were revealed, and the parametric analysis confirms that the models are accurate and have captured the essential properties of SCBA. Finally, the cross validation ensured the generalized capacity and robustness of the models. Hence, the adopted approach, i.e., MEP-based modeling with PSO, could be an effective tool for accurate modeling of the concrete properties, thus directly contributing to the construction sector by consuming waste and protecting the environment.

1. Introduction

The construction industry consumes one-third of the world’s energy and is a significant contributor of greenhouse gas emission to the environment [1]. Concrete is the most commonly used construction material. A single ton of concrete releases about 0.13 ton of carbon dioxide [2, 3]. In order to move towards sustainability, the concept of green concrete is getting popular to reduce the adverse effects of concrete. Green concrete is produced by replacing the conventional cementitious material with some waste as replacement of cement. Commonly used materials are fly ash, waste foundry sand, blast furnace slag, glass, metakaolin, rice husk ash, recycled aggregate, and bagasse ash [4]. Utilization of such materials is considered as low-carbon substitute to conventional construction materials. Sugarcane bagasse, which is an agricultural waste obtained after crushing and extraction, is used as fuel in the sugarcane industry [5]. Each ton of sugarcane generates approximately 26 percent of bagasse and 0.62 percent of residual ash [6]. The obtained ash is disposed by dumping in landfills and poses serious environmental issues [7]. Therefore, alternative and eco-friendly utilization methods of sugarcane bagasse ash (SCBA) are being discovered in the construction sector. Various research studies have concluded the viable use of SCBA in concrete as a cement replacement with a significant increase in mechanical properties of concrete. Chusilp et al. [8] reported higher compressive strength and lower permeability when concrete contained 20% SCBA by weight of cement. Sobuz [9] reported that maximum strength of SCBA concrete was obtained when cement was replaced with 10% of SCBA. Jagadesh et al. [10] reported that the strength of concrete made with 30% raw SCBA as a cement replacement reduced by almost 50%. The same authors reported about 28% increase in the strength of concrete when cement was replaced with 10% processed SCBA. The increase in strength was attributed to finer silica which reacted with calcium hydroxide to form additional CSH. Also, the finer SCBA particles filled voids and increased the packing density, which in turn increased the compressive strength of concrete. Bahurudeen et al. [11] reported higher strength of SCBA concrete as compared to normal concrete. Maximum compressive strength was achieved when cement was replaced with 10% SCBA. Strength reduction was linked with the dilution effect of the matrix caused by higher percentage replacement. Several researchers have also concluded that the utilization of SCBA also results in improved durability properties such as chloride penetration, chloride conductivity, water sorptivity, and water permeability [8, 1214]. The above discussion highlights the point that SCBA concrete behaves differently at low and high replacement levels. This behavior could be attributed to several aspects, i.e., composition and dosage of SCBA, mix proportions, and the properties and type of the concrete constituents. Therefore, it is essential to correlate and figure out the factors influencing the mechanical properties of SCBA concrete, which, in turn, will have profound effect on the construction industry.

In order to address this issue, the unique features of artificial intelligence (AI) techniques such as random forest (RF), support vector machine (SVM), artificial neural network (ANN), gene expression programming (GEP), M5P, support vector regression (SVR), and convolution neural network (CNN) have been used to develop, correlate, and find the factors influencing the mechanical properties [1519]. Zhang et al. [20] developed the RF model for the investigation of the hardened properties of synthetic-sand concrete. From results, it was found that RF showed reduced performance in comparison to other models. In a study conducted by Sun et al. [21], the authors utilized RF combined with an optimization algorithm for predicting the uniaxial compressive strength of rubberized concrete. The output of the study reported good accuracy of the model with a high correlation. Huang et al. [22] used the RF model along with beetle antenna search algorithm to predict the permeability of pervious concrete. The result of the study suggested improved performance of RF optimized model. ANN algorithm was used to model the compressive strength of lightweight concrete, foamed concrete, silica fume concrete, and high-performance concrete and elastic modulus of recycled aggregate concrete [17, 2328]. A good correlation was observed in these studies for estimating the underlying concrete properties. However, the ANN is considered as black box algorithm, since it does not consider information or physical phenomena of the related problem [29]. Moreover, due to lack of parametric studies, the ANN models may not perform well on unseen datasets [30]. Recently, the advanced GEP technique was applied to predict the mechanical properties of SCBA and waste foundry sand concrete. Sensitivity and parametric analyses were performed to assess the performance of the models developed for mechanical properties [4, 31]. In these studies, the results of the comparative study revealed superior performance of GEP over regression methods. However, the GEP was identified with certain limitations since it fails to consider a few deviating datasets for model development, thus reducing its range of applicability [4]. Such deviating datasets should be removed from both training and testing phases to improve the model performance. Furthermore, the GEP encodes only a single chromosome and is suitable for simple relationship of input and output variables [32].

Considering the above limitations of certain AI techniques, an advanced algorithm, i.e., multiexpression programming with particle swarm optimization (PSO-MEP), has been adopted to model the mechanical properties of SCBA concrete. MEP with optimization technique (PSO) has been rarely used in civil engineering field despite its distinguished features. The mechanical properties of SCBA concrete in terms of compressive strength (CS), splitting tensile strength (ST), and flexural strength (FS) were modeled using PSO-MEP to solve complex relationship. A large dataset was collected from the literature for model training and testing. The validity of the developed models was verified utilizing the results obtained from laboratory testing. Furthermore, the variable importance, parametric study, and cross validation were used to assess the robustness and accuracy of the developed models.

2. Methods and Datasets

2.1. Multiexpression Programming

A linear variant of machine learning, i.e., multiexpression programming (MEP), has been proposed recently. The individual entities can be represented as a variable length in MEP [32, 33]. The linear variants permit MEP to extricate the genotype and phenotype [34]. MEP is considered expedient over other techniques due to linear chromosomes and encoding multiple solutions in an individual chromosome. This unique feature allows to search in a wider space to gather the best possible solution. In comparison to genetic programming, the MEP applies simple decoding procedures and is given particular importance in case of unknown complexity of targeted expression [29]. MEP can handle exceptions such as invalid expressions, divide by zero, etc. MEP can handle exceptions such as invalid expressions and divide by zero and it transforms into arbitrary terminal symbol so that the process continues. This produces a margin in structure of chromosome during evaluation process [32]. The various steps involved in MEP process are shown in Figure 1. The MEP algorithm is similar to C language and pascal compiler. The outcome of the MEP process is a combination of mathematical operators or variables in a linear string of instruction form [35].

2.2. Particle Swarm Optimization

Particle swarm optimization (PSO) is a computational technique mainly used for problem optimization to enhance a solution by iterative process given a set of quality measures. This technique was developed by Kennedy and Eberhart based on motion of bird flocking and schooling fish [36]. In PSO, a process is initiated with a population of arbitrary solutions and the generations are updated to search for optimal solution. This technique is widely used for problem optimization such as forecasting the compressive strength, image contrast enhancement, and evaluating energy performance of building [37, 38]. In the present study, PSO was applied to fine-tune the hyperparameter of MEP and improve the modeling accuracy.

2.3. Modeling Database

A detailed dataset of different properties of SCBA concrete was collected from the published literature [811, 13, 14, 3960]. The collected datasets contained information about SCBA concrete at 28 days. Some of the aforementioned research studies used concrete cubes to determine the compressive strength of SCBA concrete. In order to get homogenous data, the cube strength was converted to cylinder strength according to the method suggested by Elwell and Fu [61]. The collected literature data were statistically analyzed to get the most influential parameters affecting properties of SCBA concrete. The statistical parameters of different variables used in modeling are given in Table 1 [62]. An extensive study of design codes revealed that different models are available correlating the mechanical properties of normal concrete with compressive strength [6367]. Therefore, the water to cementitious ratio (W/C), proportions of bagasse ash (SCBA%), fine aggregate content (FA), cement content (CC), and quantity of coarse aggregate (CA) are chosen as input for prediction of SCBA concrete mechanical properties. The formulation of compressive strength (CS), splitting tensile strength (ST), and flexural strength (FS) of SCBA concrete is considered to be a function of the following variables:

2.4. Modeling Parameters for MEP

For developing a generalized relationship, several fitting parameters are required for MEP. The chosen parameters for MEP modeling are presented in Table 2. Basic mathematical operators were considered to get simple expressions. The trial and error method was adopted to get the fitting parameters [68]. The population size was used to specify the number of programs required in the population. High population can lead to complex and long convergence time and often causes overfitting problem beyond specified limit. Moreover, an algorithm run with a large number of generations could lead to a model with minimum error. Several combinations of parameters were initiated and the best possible grouping was selected based on the model performance.

2.5. Performance Evaluation

The performance of the developed PSO-MEP model was assessed by measuring various statistical indicators including correlation coefficient (R), root mean squared error (RMSE), Nash–Sutcliffe efficiency (NSE), mean absolute error (MAE), relative root mean squared error (RRMSE), relative squared error (RSE), and performance index (ρ). Moreover, another measure to reduce the model overfitting is to select the best model by minimizing the objective function (OF) as suggested by Gandomi et al. and Azim [34, 69]. The same approach has been applied in this study, and OF is termed as fitness function. The mathematical expressions for the statistical indicators are shown below from equations (2) to (9). The high values of R and NSE and low values of RMSE and MAE indicate better performance. The indicator R quantifies the linear relationship between input and output [27], and R value more than 0.8 signifies excellent correlation among predicted and actual data [70]. However, it alone cannot be considered to judge the efficiency of a model. Despotovic et al. [71] highlighted that a model can be considered excellent if the value of RRMSE is between 0 and 0.10 and good if the values are between 0.11 and 0.20. The minimum and maximum value of NSE is negative infinity and 1, respectively, with 1 showing the best output. The values of ρ and OF range from 0 to positive infinity with a value near to zero representing a good model. It can be noted that the OF taken into account the effect of RRMSE, R, and relative percentage of data in different sets. Hence, low OF value shows superior performance of a model.where show the number of data points, predicted data, measured data, mean of predicted data, and mean of measured data, respectively. T and TE represent the training and testing datasets, respectively.

2.6. Hyperparameter Tuning and K-Fold Cross Validation

Fine-tuning of hyperparameters is a major concern in machine learning-based modeling. Various researchers used different optimization techniques for hyperparameter tuning such as beetle antennae search [22, 72, 73] and grid search method [74]. In our study, particle swarm optimization (PSO) was employed for hyperparameter tuning to improve the accuracy of the model. Firstly, the dataset was divided into 70% and 30% for model training and testing, respectively. Then k-fold cross validation was applied to assess the hyperparameter tuning process by PSO. The k-fold method divides the actual data to k subclasses. Moreover, the efficiency of the 10-fold cross validation method is reported in the literature [75, 76]. Among all the ten subsets, each subset was used for validation and the same method was repeated for all the remaining subsets. Consequently, the optimized MEP model and the associated optimized hyperparameters were obtained after 10 rounds. After getting the optimum structure of MEP by PSO, the result of training and testing dataset was evaluated employing statistical indicators. Finally, 10-fold cross validation was used again to ensure the generalized capability of PSO-MEP and output was expressed in terms of mean accuracy. Figure 2 shows the hyperparameter tuning process for MEP with the help of PSO for both training and testing.

3. Experimental Investigation

3.1. SCBA Processing

The sugarcane bagasse ash (SCBA), resulting from burning of bagasse (as a fuel), was collected from a sugar industry located in Malakand, Pakistan. It has been reported in the literature that the presence of fibrous and unburnt content in raw bagasse ash decreases the pozzolanic activity and also elevates the loss on ignition. Removal of such particles, proper characterization, and grinding up to cement fineness significantly increase its pozzolanic activity [11, 77]. In our study, the collected SCBA was sieved from #200 sieve to remove undesirable particles and subsequently grinded to reduce the particle size. Grinding was carried out in ball mill machine with ceramic balls as grinding media. The grinding media to SCBA ratio of 5 by weight was kept constant, and the machine was operated at 100 rpm [78]. Different SCBA samples were obtained at a grinding duration of 15, 30, 45, and 60 minutes. Blaine fineness values were determined according to ASTM C204 in order to obtain the effect of grinding on particle size.

The chemical composition of grounded SCBA was evaluated through X-ray fluorescence (XRF). The composition is given in Table 3. It can be inferred from XRF results that the quantity of silica, alumina, and iron oxide is above 70%, meeting the chemical requirement of a pozzolan according to ASTM C618-05 standard.

Scanning electron micrographs of SCBA are shown in Figure 3. Images were taken at different magnification ranging from X500 to X5000. In the micrographs, the heterogeneous nature of SCBA is prominent. The SCBA exhibited various shapes such as elongated, needle, flat, oval, and irregular. According to available literature [79], the irregular shape particles are mainly rich in silica. The size of needle and oval shape particles is about 50 μm. Furthermore, voids over the surface ranging from 5 μm to 10 μm are visible in the form of black spots. Overall, the observed size of different particles ranges from 5 μm to 50 μm.

3.2. Mix Proportions and Properties of SCBA Concrete

Experimental testing of SCBA concrete was conducted to check the performance of the model required for validation purpose. Concrete specimens were casted at room temperature of 25°C, and comparison of fresh and hardened properties was made between concrete made with bagasse ash (BC) and control specimens (CM). Different dosages of SCBA, i.e., 0–40%, were incorporated in concrete as cement replacement. The desired target strength was formulated based on published data as adamant variation was observed. The detailed mix design with the formulation is depicted in Table 4.

For the validation of the PSO-MEP model, concrete specimens, i.e., cylinders and 4” × 4” × 20″ beams, were prepared with different proportions of SCBA and tested for compressive strength (CS), splitting tensile strength (ST), and flexural strength (FS), respectively, at the curing age of 28 days. ASTM standards C39, C496, and C293 were, respectively, followed for compressive, splitting tensile, and flexural strength of the CM and BC.

4. Results and Discussion

4.1. Mechanical Properties of SCBA Concrete

The results of mechanical properties, i.e., compressive strength (CS), splitting tensile strength (ST), and flexural strength (FS), of SCBA concrete were determined in laboratory by casting concrete cylinders and beams with varying proportions of SCBA (0% to 40%), as presented in Table 5. It can be observed that strength increased up to 10% SCBA and then consistently decreased at higher SCBA level. The maximum strength gained is at 10% replacement. The strength gain at 10% SCBA may be related to the pozzolanic reaction resulting in additional calcium silicate hydrate (CSH). For higher replacement level, the decrease in strength was found to be 6.5%, 17.3%, and 30.3% for 20BC, 30BC, and 40BC, respectively. This decrease in strength may be attributed to unavailability of the adequate amount of calcium hydroxide.

Similar results were observed for splitting tensile strength and flexural strength as illustrated in Table 5. For 10% and 20% replacement of SCBA, the increase in tensile strength as compared to control concrete was 25.3% and 15.8%, respectively. This shows that the maximum tensile strength was attained at 10% addition of SCBA as cement replacement. For 30% and 40% SCBA replacement level, the tensile strength decreased by 7.9% and 23.8%, respectively, as compared to CM. For the case of flexural strength, the maximum strength was also achieved at 10% SCBA. The flexural strength at higher replacement level (20%, 30%, and 40% SCBA) reduced by 15.5%, 28.8%, and 42.5%, respectively. According to available literature, the increased tensile and flexural strength at 10% SCBA may be due to the microfibrous nature of SCBA, which is related with CSH formation, and also due to the formation of aluminates, resulting in needle-like structure [80, 81]. The interlocking of these needles takes place between hydrated paste and may directly enhance the tensile and flexural strength. In short, the enhanced properties may be due to formation of more hydrated products, less porous structure of concrete made with SCBA, and the enhanced interfacial transition zone (ITZ) [80, 82, 83].

4.2. Formulation of Mechanical Properties with PSO-MEP

The results obtained from PSO-MEP for compressive strength (CS), splitting tensile strength (ST), and flexural strength (FS) are interpreted to get the empirical mathematical expressions for the prediction of aforementioned properties based on five input variables. The derived equations are shown as equations (10), (11), and (12) for CS, ST, and FS, respectively. A comparative graph of experimental and predicted CS is presented in Figure 4 for training, testing, and validation. The expressions for regression lines are also shown. For an ideal situation, it is known that the slope of the line should be nearly equal to 1. It can be deduced from Figure 4 that the developed PSO-MEP model considered the effect of input variables and retains a strong correlation between experimental and predicted data as evident from the slope, i.e., 0.8951, 0.9315, and 0.9014 for training, testing, and validation, respectively.where

A similar comparison has been drawn for the tensile strength (ST) output as shown in Figure 5. It can be seen that the model exhibited an excellent correlation among experimental and predicted data to estimate ST. The respective slopes of the regression line are close to ideal fit, i.e., 0.9351, 0.8903, and 0.9273 for training, testing, and validation. Similar to CS, the model for ST performs exceptionally well on training dataset revealing that the issue of overfitting by the model has been reduced to a larger extent. Moreover, the performance and accuracy of a model depend on the number of data points incorporated in the model [84]. In this study, 110 data points have been selected to model ST; therefore, an accurate model with minimum error has been achieved.

The PSO-MEP model results for flexural strength (FS) are graphically presented in Figure 6. During model training, testing, and validation, the slope of the regression line was observed to be 0.9494, 0.9026, and 0.9332. Compared with the models for CS and ST, an excellent estimate is observed for experimental and predicted data point as illustrated in Figure 6. The model performs exceptionally well for training and testing data.

4.3. Model Evaluation by Statistical Measures

The reliability of a model depends on the amount of data used for model development. The literature survey recommended that the ratio of number of data points to the number of input variables for both training and testing should be greater than 5 [85]. For model training, the aforementioned ratio is 11.8, 13.8, and 8.2 for CS, ST, and FS, respectively. For model testing, the values are 6.2, 6.6, and 5.7 for CS, ST, and FS, respectively. The performance of the developed models was evaluated by various statistical criteria such as RMSE, NSE, RSE, RRMSE, OF, ρ, MAE, and R. The values of these indicators for CS, ST, and FS are given in Table 6 for training, testing, and validation. It can be observed from Table 6 that models exhibit a strong correlation as evident by the R value which is 0.91, 0.90, and 0.91 for training and 0.94, 0.92, and 0.91 for testing of CS, ST, and FS, respectively. The maximum and minimum values of NSE are 0.89 and 0.87 for CS, 0.91 and 0.85 for ST, and 0.86 and 0.87 for FS models, respectively. The values of RMSE and MAE are considerably low for the three datasets which highlighted the generalized capability and high accuracy of the models. Based on RMSE, the model for ST can be categorized as excellent, as the values for all the three datasets are 2.43, 2.65, and 3.25, respectively. It can be deduced from results that for all models, MAE lies in the good range from 1.45 to 3.98. Furthermore, the OF values for CS, ST and FS are 0.036, 0.031, and 0.052, respectively. All these values are close to zero, indicating the accurate performance and further validating that the overfitting problem has been suitably addressed by the models. For all the developed models, the RRMSE ranged from 0.04 to 0.16, thus highlighting the accuracy of the model in predicting the mechanical properties of SCBA concrete. In order to infer the absolute error, the data points are plotted in Figure 7 showing the error among actual and model simulated data. The mean absolute error for CS, ST, and FS is 2.87, 0.405, and 0.675, respectively. The minimum and maximum absolute errors are 0.1 and 7.76 for CS, 0.08 and 2.15 for ST, and 0.075 and 1.95 for FS, respectively. It is worth mentioning that almost 80% of results for CS, ST, and FS have error less than 3, 0.5, and 0.6, respectively.

The criteria for external validation of the models are given in Table 7. It has been suggested that regression line slope, i.e., k and k′, passing through the origin should be nearly equal to 1 [86]. Roy and Roy [87] reported that criteria for external predictability of a model are satisfied when the indicator Rm is greater than 0.5. It can be observed from Table 7 that all the three models (CS, ST, and FS) satisfy the conditions for external predictability.

4.4. Model Cross Validation Results

The 10-fold cross validation was applied to evaluate the CS, ST, and FS models, and the results are graphically shown in Figures 8 and 9 for R and RMSE, respectively. A variation in the results can be observed at individual level as depicted in the figure. However, it demonstrated a good mean accuracy. The average R value obtained for CS, ST, and FS is 0.85, 0.89, and 0.85, respectively. In all the 10-fold cross validations, the maximum and minimum R values of 0.72 and 0.91, respectively, were achieved by ST. Similarly, the mean RMSE values of 4.54, 3.89, and 4.78 were accomplished by CS, ST, and FS, respectively. For individual subset, the lowest RMSE, i.e., 1.86, was also attained by ST. Overall, the results from 10-fold cross validation shows the accurate performance, generalized capability, and robustness of the PSO-MEP models.

4.5. Variable Importance and Parametric Analysis

Variable importance is a process to find out the most influencing input variables affecting the targeted output. The most sensitive input parameters and their relative contribution to output were determined, and the results are illustrated in Figure 10. The result shows that cement content is the most important variable contributing 55% to mechanical properties of SCBA concrete. Similarly, water-cement ratio and amount of coarse aggregate turned out to be important variables with 17.15% and 16.97% contribution to the output. The result further reveals that quantity of fine aggregate is the least important parameter affecting the mechanical properties of SCBA concrete.

Parametric analysis was performed to assess the variation of the model output with every single input variable. This process is recommended in research studies to determine the effect of all the physical phenomena and inputs. In this method, all the variables were kept constant at their mean values and the variation of the model output is plotted with a single input variable. The same procedure was applied for the individual input parameter. Figure 11 shows the parametric analysis results for the developed CS model only as similar patterns were obtained for other mechanical properties (ST and FS). Therefore, parametric study results are discussed in detail for CS in the following.

It is a known fact that an increase in water-cement ratio decreases the strength of concrete [84, 88]. It can be seen form Figure 11(a) that an increase in W/C resulted in a consistent decrease in compressive strength. The effect of SCBA% on the mechanical properties of SCBA concrete depends on physical and chemical composition and replacement percentage of SCBA [11]. It can observed in Figure 11(b) that the compressive strength of SCBA concrete increased up to a certain level and then decreased with increase in the level SCBA%. It can be deduced from the figure that maximum strength has been attained at 10% SCBA replacement. A similar trend was also observed for experimental testing of SCBA concrete as described in Section 4.1. Hence, the results of parametric analysis are in close agreement with laboratory testing where maximum strength was achieved at 10% SCBA. Similar findings were reported in [911] which showed that 10% SCBA replacement attained higher strength.

Cement is the principal cementitious material in concrete, and the increase in the cement content enhances the mechanical properties of concrete. A similar trend can also be seen in Figure 11(c) where the compressive strength linearly increased with increase in cement content. The higher cement content produces more calcium silicate hydrate (CSH) which forms a dense structure, thereby increasing the compressive strength. Figures 11(d) and 11(e) illustrate the variation of compressive strength with fine and coarse aggregate content, respectively. Both figures demonstrated that CS decreased with the increase in FA and CA content. The aggregates are inert materials and are used to provide volume stability to concrete. The quantity of aggregates affects the mechanical properties of concrete. However, keeping all the quantities constant in a mix, the strength of concrete decreases with increase in the quantity of aggregate. Similar results were also observed in the current study.

From the aforementioned discussion, it can be concluded that the developed PSO-MEP model has successfully incorporated the effect of all input variables, specifically the complex physical behavior of SCBA, thus making it more suitable for estimation of complex problems.

5. Conclusion

This study adopted the two-fold objective. Firstly, the compressive strength, splitting tensile strength, and flexural strength of SCBA concrete were modeled by utilizing multiexpression programming (MEP). The particle swarm optimization (PSO) was employed to tune the hyperparameter of the model. The proposed model was developed and formulated based on extensive literature data. Secondly, sugarcane bagasse ash (SCBA) was characterized, optimized, and used in different proportions (10%, 20%, 30%, and 40%) as a partial replacement with cement. SCBA concrete specimens were prepared and tested for mechanical properties, and the results were used for model validation. The performance and accuracy of the final models were evaluated with the help of statistical indicators, i.e., RMSE, NSE, RSE, RRMSE, OF, ρ, MAE, and R. The results obtained from the developed models exhibited an excellent correlation with the experimental data with R value above 0.9, MAE and RMSE below 5, and OF values close to zero for CS, ST, and FS models. The developed PSO-MEP models also satisfied the criteria for external validation available in the literature. The variable importance and parametric analysis revealed that the developed model has taken into account the effect of all the inputs. The final outcome of the model was also cross verified with the 10-fold validation; the results ensured that the models produced generalized outcome, and the overfitting issue has also been addressed. It is obvious from the current study that utilization of different wastes is indispensable for sustainability viewpoint and machine learning models play a crucial role in its success.

Data Availability

The data used in this study were collected from the published literature and are available from the corresponding author upon request.

Conflicts of Interest

The authors declare that they have no conflicts of interest.