Nanostructured and Spiky Gold Shell Growth on Magnetic Particles for SERS Applications
Next Article in Special Issue
Impact of Tm3+ and Tb3+ Rare Earth Cations Substitution on the Structure and Magnetic Parameters of Co-Ni Nanospinel Ferrite
Previous Article in Journal
Effect of Random Nanostructured Metallic Environments on Spontaneous Emission of HITC Dye
Previous Article in Special Issue
Magnetite-Arginine Nanoparticles as a Multifunctional Biomedical Tool
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Functional Sr0.5Ba0.5Sm0.02Fe11.98O4/x(Ni0.8Zn0.2Fe2O4) Hard–Soft Ferrite Nanocomposites: Structure, Magnetic and Microwave Properties

by
Norah A. Algarou
1,2,
Yassine Slimani
1,*,
Munirah A. Almessiere
1,2,*,
Ali Sadaqat
3,
Alex V. Trukhanov
4,5,6,*,
Mohammad A. Gondal
7,
Abbas S. Hakeem
8,
Sergei V. Trukhanov
5,6,
Maksim G. Vakhitov
5,9,
Denis S. Klygach
5,9,
Ayyar Manikandan
10 and
Abdulhadi Baykal
11
1
Department of Biophysics, Institute for Research and Medical Consultations (IRMC), Imam Abdulrahman Bin Faisal University, P.O. Box 1982, Dammam 31441, Saudi Arabia
2
Department of Physics, College of Science, Imam Abdulrahman Bin Faisal University, P.O. Box 1982, Dammam 31441, Saudi Arabia
3
Department of Mechanical and Energy Engineering, College of Engineering, Imam Abdulrahman Bin Faisal University, P.O. Box 1982, Dammam 31441, Saudi Arabia
4
Department of Electronic Materials Technology, Institute of New Materials and Nanotechnology, National University of Science and Technology MISiS, 119049 Moscow, Russia
5
Department of Design and Manufacture of Radio Equipment, School of Electronic Engineering and Computer Science South Ural State University, 454080 Chelyabinsk, Russia
6
Laboratory of Magnetic Films Physics, SSPA “Scientific and Practical Materials Research Centre of NAS of Belarus”, 220072 Minsk, Belarus
7
Laser Research Group, Department of Physics & Center of Excellence in Nanotechnology, King Fahd University of Petroleum and Minerals (KFUPM), P.O. Box 5047, Dhahran 31261, Saudi Arabia
8
Center of Research Excellence in Nanotechnology (CENT), King Fahd University of Petroleum and Minerals (KFUPM), P.O. Box 5047, Dhahran 31261, Saudi Arabia
9
Laboratory “Electromagnetic Compatibility”, Centre of Collective Usage, Federal State Autonomous Educational Institution of Higher Education ‘Ural Federal University Named after the First President of Russia B.N. Yeltsin’, 620002 Ekaterinburg, Russia
10
Department of Chemistry, Bharat Institute of Higher Education and Research (BIHER), 10 Bharat University, Chennai 600073, India
11
Department of Nanomedicine Research, Institute for Research and Medical Consultations (IRMC), Imam Abdulrahman Bin Faisal University, P.O. Box 1982, Dammam 31441, Saudi Arabia
*
Authors to whom correspondence should be addressed.
Nanomaterials 2020, 10(11), 2134; https://doi.org/10.3390/nano10112134
Submission received: 24 September 2020 / Revised: 21 October 2020 / Accepted: 21 October 2020 / Published: 27 October 2020
(This article belongs to the Special Issue Functional Nanomagnetics and Magneto-Optical Nanomaterials)

Abstract

:
This paper reports the correlation between the composition of the functional Sr0.5Ba0.5Sm0.02Fe11.98O19/x(Ni0.8Zn0.2Fe2O4) hard–soft nanocomposites (SrBaSmFe/x(NiZnFe) NCs), where 0.0 ≤ x ≤ 3.0, and their structural features, magnetic, and microwave properties. SrBaSmFe/x(NiZnFe) hard/soft ferrite NCs are produced using the one-pot citrate combustion method. According to the XRD analysis, all samples showed the co-existence of both SrBaSmFe and NiZnFe phases in different ratios. Magnetic properties are measured in a wide range of magnetic fields and temperatures (10 and 300 K) and correlated well with the composition of the investigated samples. The microwave properties (frequency dispersions of the magnetic permeability, and electrical permittivity) are discussed by using the co-axial method in the frequency range of 0.7–18 GHz. Non-linear dependences of the main microwave features were observed with varying of composition. The microwave behavior correlated well with the composite theory. These results could be used in practice for developing antenna materials.

1. Introduction

The development of new functional composites with controllable magnetic and microwave properties is one of the important tasks of modern applied physics. Nowadays, functional hard–soft magnetic composites are attracting the attention of scientists; spinel ferrites and composites based on them have had great contributions in many fields, such as materials for catalysis [1,2], targeted drug delivery [3], microwave, gas sensors [4], magneto-optical data storage [5], medicines, cancer treatment, telecommunications, photoactive materials, and photo-catalysts. Microwave absorption is one of the most promising directions of complex iron oxides [6,7] because its high saturation magnetization (Ms), large coercivity (Hc), and strong coupling between magnetic phases. This opens for new perspectives for the integration of the magnetic materials in electronics [8].
Kneller et al. [9] have proposed that permanent magnets could be produced based on composite materials comprising two appropriately dispersed hard and soft magnetic phases that are mutually exchange-coupled. The large coercivity (provided by hard magnetic phase) and the high saturation magnetization (provided by soft magnetic phase) of magnetic hard/soft ferrites composites can be achieved when the exchange coupling is performed [10,11,12,13]. Many researchers have reported the exchange coupling behavior for some multilayer and metal alloy systems like Nd–Fe–B [14], SmCox–Co [15], Pr2Fe12B [16], and Sm–Co/Fe [17]. There are many kinds of hard/soft ferrite composites that have attracted the interest of researchers. For example, ferrite–polymer composites such as Ni0.5Zn0.5Fe2O4/BaFe12O19@polyaniline composites have been synthesized and investigated [6]. Additionally, the quite popular core-shell structures of NiFe2O4/SrCo0.2Fe11.8O19 [18] and Mn0.6Zn0.4Fe2O4@Sr0.85Ba0.15Fe12O19 [19] have been also explored. Ceramics-based composites such as SrTb0.01Tm0.01Fe11.98O19-AFe2O4 (A = Co, Ni, Zn, Cu and Mn) [20], BaFe12O19/CoFe2O4 [12], Sr0.3Ba0.4Pb0.3Fe12O19/(CuFe2O4)x [7] (Ba0.5Sr0.5Fe12O19)1−x(CoFe2O4)x [21], SrFe12O19/Ni0.7Zn0.3Fe2O4 [22], Li0.3Co0.5Zn0.2Fe2O4/SrFe12O19 [23], and fiber-based composites such as SrFe12O19/Ni0.5Zn0.5Fe2O4 nanofibers [11] have been intensively investigated. Great attention has been paid to hard/soft magnetic nanocomposites (NCs) due to the significant improvement of their overall magnetic properties. It has been verified that the composition, microstructure, grain size, and strength of magnetic interaction greatly affect the exchange coupling between hard and soft ferrite phases [7,12]. The structural and magnetic properties of these NCs could be improved by optimal calcination conditions, appropriate hard–soft ratios, and well-exchange coupling between hard and soft ferrite phases [23,24,25,26]. The achievement of well-exchange coupling in hard/soft ferrite nanocomposites is still a challenging task to be accomplished [27]. Accordingly, it is very important to synthesize composite materials that display well-exchange coupling behavior [28,29,30].
Separate hard and soft ferrites are favorable for outstanding applications [31]. Soft spinel ferrites with a low anisotropic value are suitable for, e.g., microwave applications [32]. On the other hand, hard ferrites such as BaFe12O19 have a high ferromagnetic resonance frequency (~35 GHz) and a high magnetocrystalline anisotropy, making them suitable for W-band applications [33]. Consequently, combinations of low anisotropic soft ferrite and high anisotropic hard ferrite are largely used as permanent magnets, as well as for different microwave device applications such as functional devices (circulators and inventors) and antennae [34,35]. Radar absorbing materials (RAM) have excellent microwave absorbing properties due to their high range of 8.2–12.4 GHz [36]. However, a large absorption peak, thin absorption layer, and wide working frequency range cannot be achieved by using a single material of an ideal radar absorber [8,37]. Nanocomposites could help to construct unified systems comprising hard and soft ferrite phases, where the properties would be exclusive and complimentary [21]. Magneto-dielectric composites have a high permeability and a highly permittie nature due to the exchange coupling effect that could substitute dielectric substrates for antenna miniaturization. However, some composites are scarcely used because of their high frequency range between 12 and 18 GHz [38].
There are two ways to develop hard–soft ferrite nanocomposites. One of them is concerned with varying the chemical composition of the initial components. The second one is concerned with varying the mass ratio of soft and hard phases. In this study, SrBaSmFe/x(NiZnFe) hard/soft ferrite NCs with varying hard/soft phases ratios of 1:x (where 0.0 ≤ x ≤ 3.0) were synthesized. The structural, magnetic, and microwave properties were deeply investigated. The correlation between composition, structural features, microwave properties, and magnetic properties of the composites is discussed in terms of coupling strength between different constituting phases.

2. Materials and Methods

Hard/soft ferrite SrBaSmFe/x(NiZnFe) (0.0 ≤ x ≤ 3.0) NCs were prepared via the one-pot citrate combustion methodology, as shown in Figure 1 [39]. Firstly, SrBaSmFe and NiZnFe were prepared individually through the sol–gel auto-combustion approach. In order to prepare SrBaSmFe, a specific amount of Sr(NO3)2, Fe(NO3)3.9H2O, Sm(NO3)3·6H2O, and C6H8O7 were dissolved in 50 mL of deionized (DI) water under continuous stirring at 90 °C for 45 min to get the SrBaSmFe solution. For the particular synthesis of the NiZnFe solution, Ni(NO3)2·6H2O, Zn(NO3)2·6H2O, Fe(NO3)3·9H2O, and C6H8O7 were dissolved together in 50 mL of DI water under stirring at 85 °C for 45 min. The pH of both solutions was regulated at 7 with an ammonium hydroxide solution (NH4OH) while tuning the temperature to 180 °C for 50 min and then raising it to 370 °C to get black ash. The final products of SrBaSmFe and NiZnFe were calcinated for 6 h at 1000 and 950 °C, respectively.
The SrBaSmFe/NiZnFe hard/soft ferrite NCs with different fractions were produced by mixing the initial solutions of SrBaSmFe and NiZnFe under continuous stirring at 85 °C for 35 min. The pH of the hard/soft solution was modified with an ammonium solution to reach 7. At that time, the temperature was increased to 180 °C for 50 min and then raised again to 350 °C until a black powder was obtained. The resulting powders were calcinated at 1000 °C for 6 h to get the final hard/soft nanocomposites.
The hard/soft ferrite NC structure was examined by employing XRD (X-ray powder diffraction) Rigaku D/MAX-2400 (Cu Kα). The morphology was observed via FE-SEM (Lyra3, Tescan, Brno, Czech Republic) coupled with an energy-dispersive X-ray (EDX) system. Transmission electron microscope (TEM) and high-resolution transmission electron microscope (HR-TEM) (FEI Titan ST Microscopes) were employed to approve the morphology and structure. A vibrating sample magnetometer (VSM) was used to get the magnetic measurements of the products. Microwave parameters (permittivity and permeability) were estimated as frequency dispersions of the real and imaginary parts from direct S-parameters measurements. The S-parameters of the transmission line were analyzed by means of a vector network analyzer (R&S model ZVA24) in the 8–12 GHz range. S11 parameters were measured in two regimes: Firstly, in a short circuit regime and secondly, in a matched-load regime. The measured values were used to calculate the frequency dispersions of the magnetic permeability and electrical permittivity (real and imaginary parts). The measurement procedure was reported in [40]. Full two-port calibration was initially performed on the test setup to remove errors due to the directivity, source match, load match, isolation, and frequency response in both the forward and reverse measurements. The measured reflection coefficient (S11) and transmission coefficient (S21) of the samples were converted into real and imaginary parts of permeability; the permittivity ( μ ˙ and μ ˙ ) and permeability ( ε ˙ and ε ˙ ) of the material were calculated by the Nicholson–Ross–Weir algorithm from the S-parameters recorded as a function of frequency.

3. Results and Discussion

The main idea of the conducted research was the observation and explanation of the correlation between composition (ratio between soft and hard phases), crystal structure, microstructural features, magnetic properties, and microwave properties in the composites. The correlation between structural parameters and magnetic properties for both magnetic phases and the existence of outstanding magnetic exchange-coupling between the phases could open perspectives for the observation of any phenomena in magnetic and microwave properties.

3.1. Microstructure

The structural analyses of SrBaSmFe/x(NiZnFe) (0.0 ≤ x ≤ 3.0) hard/soft ferrite NCs were implemented through the investigation of XRD powder patterns. Figure 2a presents the XRD patterns of pure SrBaSmFe and NiZnFe separately. These patterns show the characteristics peaks of M-type hexaferrite for the SrBaSmFe sample and a cubic spinel structure for the NiZnFe product. No undesired impurity was observed in either sample. On the other hand, Figure 2b presents the XRD patterns of various hard/soft SrBaSmFe/x(NiZnFe) NCs where x = 1.0–3.0. XRD patterns for all compositions showed the successful co-formation of M-type hexaferrite and cubic spinel phases within the nanocomposite, and no impurity was discerned. It is obvious that there is a disparity in the intensity of indexed peaks of hard/soft ferrite NCs because of the gradual increase in the spinel content. This can be attributed to the effectiveness of the synthesis method, which allowed for homogenization between the hexagonal and spinel phases. The structural parameters and the fraction percentage of various hard/soft ferrite SrBaSmFe/x(NiZnFe) (0.0 ≤ x ≤ 3.0) NCs were determined via Match 3! and Full Proof software (Table 1). It was noticed that the lattice constant ‘a’ of the hard ferrites increased with the addition of soft ferrite, while the lattice parameter ‘c’ of hard ferrite and ‘a’ of soft ferrite fluctuated, maybe due to the alteration in the solubility between the soft and hard ferrite [41]. The average crystallite sizes (D) of SrBaSmFe and NiZnFe were calculated by applying the Scherrer equation (DXRD = Kλ/βcosθ, where K is a shape constant, λ is the wavelength of CuKα radiation (1.5406 Å), and β is the peak width at half maximum intensity) on the intense peaks of hard and soft ferrites. It was noticed that the crystallite size of the hard phase was around 45% larger than that of the soft phase. The crystallites size varied from 50 to 83 nm and from 21 to 50 nm for the hard and soft products, respectively.

3.2. FESEM and TEM Analysis

The analyses of the microstructure of pure SrBaSmFe, pure NiZnFe, and various hard/soft ferrite NCs of SrBaSmFe/x(NiZnFe), where x = 1.5 and 2.5, were performed with the FE-SEM technique (Figure 3). The images revealed that the morphology of NiZnFe consisted of aggregated grains with spherical shapes. Meanwhile, the SrBaSmFe NCs exhibited randomly oriented hexagonal platelets grains. The FE-SEM images of hard/soft ferrite SrBaSmFe/x(NiZnFe) NCs with x = 1.5 and 2.5 disclosed hexagonal plates decorated by clusters of spherical grains. It was obvious that the morphology of hard/soft ferrite NCs was changed upon the increase of the content of spinel ferrite to become most hexagonal platelets covered by assembled spherical grains. The EDX and elemental mapping of hard/soft ferrite SrBaSmFe/x(NiZnFe) NCs with x = 1.5 and 2.5 were carried out and are presented in Figure 4. Theses analyses showed the existence of various required elements and verified the successful formation of the desired compositions. This proved the efficiency of the used preparation method. To further confirm the formation and the morphology of hard/soft ferrite SrBaSmFe/x(NiZnFe) NCs, TEM, and HR-TEM investigations for x = 1.5 and 2.5 NCs were performed (Figure 5). The TEM images demonstrated the combination of hard and soft phases. The interplanar fringes provided by HR-TEM images were consistent with the hard and soft phases, which confirmed the coexistence of both hard and soft phases.

3.3. VSM Investigation

Figure 6 provides the variations of magnetization (M) as a function of an applied magnetic field (H), as found by exposing samples of SrBaSmFe and NiZnFe to a magnetic field H = ±70 kOe. The magnetic measurements were carried out at two measured temperatures of T = 300 and 10 K. The M(H) plots of pure NiZnFe nanoparticles (NPs) showed roughly S-shaped behavior without coercivity (Hc) and remnant magnetization (Mr), thus revealing that these NPs were superparamagnetic (SPM) at both temperatures. The Ms values for NiZnFe NPs were about 76.6 and 121.9 K at 300 and 10 K, respectively. However, pure SrBaSmFe hexaferrite (HF) displayed ferrimagnetic (FM) behavior at both 300 and 10 K. Indeed, SrBaSmFe HFs disclosed Hc values of 4852 and 3486 Oe at 300 and 10 K, respectively, and its Ms and Mr values were about 67.0 and 39.6 emu/g at 300 K and around 101.6 and 59.4 emu/g at 10 K. The very high Ms values of soft magnetic NiZnFe nano-spinel ferrites and the large coercivity of hard magnetic SrBaSmFe HFs could suggest that combining these two phases would be appropriate for developing well exchange-coupled nanocomposites.
In this work, the exchange-coupling behavior in the produced products of Sr0.5Ba0.5Sm0.04Fe11.96O19/x Ni0.8Zn0.2Fe2O4 (or SrBaSmFe/xNiZnFe for brevity), where x content is equal to 0.0–3.0, were carefully investigated through VSM measurements. Figure 7 presents the M(H) curves of various produced products by exposing them to H = ±70 kOe at 300 K and 10 K. All produced products exhibited FM characteristics at both 300 and 10 K. Ms magnitudes were in the interval of 47.3–66.3 emu/g at 300 K and of 57.1–86.4 emu/g at 10 K. Mr values were in the interval of 10.1–26.7 emu/g at 300 K and of 17.0–36.6 emu/g at 10 K. Hc magnitudes ranged between 155 and 2103 Oe at 300 K and between 319 and 2158 Oe at 10 K. The magnetizations were increased for various prepared products at 10 K in comparison to those at 300 K. In fact, once a negative impact of thermal energy on the quantitative organization of magnetic moments considerably reduces, the recorded magnetization certainly increases [42,43]. This largely eminent aspect that is evidenced from the various M(H) hysteresis loops of produced products is their shapes. Indeed, the different produced products illustrated the presence of a “kink” in the variation of M(H) curves, as displayed in Figure 7b,d. Such an observed kink reflects uncompleted exchange coupling among the two phases; hence, the hard and soft phases are separately switching [44]. Consequently, an overlapping of two loops resulting from separated soft and hard phases will be perceived [45].
The different magnetic parameters were deduced for various products. For better presentation, the progressions in Mr, Ms, and Hc values are presented against the various amounts of the NiZnFe soft phase in Figure 8. The Ms values were estimated from the extrapolation of M against 1/H2 plots, as reported in the following references [46,47,48]. At both 300 and 10 K, the highest Ms, Mr, and Hc magnitudes belonged to SrBaSmFe/1.0(NiZnFe) product (i.e., x = 1.0) and continuously reduced with rising the weight fraction of the NiZnFe soft phase. For this product, Ms,max and Mr,max were equal to 66.3 and 26.7 emu/g at 300 K and 86.4 and 36.6 emu/g at 10 K, respectively. The larger Hc magnitudes were about 2103 and 2158 Oe at 300 and 10 K, respectively. The smallest Ms, Mr, and Hc parameters were registered for SrBaSmFe/3.0(NiZnFe) product (i.e., x = 3.0). This nanocomposite sample had Ms = 47.3 and 57.1 emu/g at room temperature (RT) and 10 K, respectively. Mr,min were nearly 10.1 and 17.0 emu/g at RT and 10 K, respectively. Hc reduced sharply to values of 155 and 319 Oe for the x = 3.0 product. Generally, two chief interactions prevail in hard/soft products; those among hard/hard grains and soft/soft grains that are referred as dipolar interactions and those between hard/soft grains that are denoted as exchange-coupling interactions [49,50]. When the dipolar interactions are irrelevant, the magnetization is chiefly governed by exchange interactions and magneto-crystalline anisotropy. Because of rising the soft composition within the products, the dipolar interactions come to be more important. As consequence, the Ms, Mr, and Hc values of products will diminish.
The magneton numbers ( n B ) were determined for hard SrBaSmFe and soft NiZnFe phases from the common formula n B = m o l e c u l a r   w e i g h t × M s / 5585 [51]. Magneton numbers were calculated as 3.22 μB (at 300 K) and 5.12 μB (at 10 K) for the NiZnFe soft spinel ferrite. On the other hand, n B values were found to be around 13.06 and 19.80 μB for SrBaSmFe HFs at 300 and 10 K, respectively. Nevertheless, this simple formula could not be used for the produced products since they comprised the contributions of resultant magnetic moments coupled with the fractions (fMW) of NiZnFe and SrBaSmFe phases in the products. Accordingly, to determine accurately the total magneton numbers for the produced products, the following relation was employed:
n B = f M W , N i Z n F e n B , N i Z n F e + ( 1 f M W , N i Z n F e ) n B , S r B a S m F e
At RT, the determined magneton number decreased linearly from a maximum value n B = 8.14   μ B that belonged to the SrBaSmFe/(NiZnFe)1.0 product to a minimum value n B = 5.68   μ B for the SrBaSmFe/(NiZnFe)3.0 product. At T = 10 K, n B magnitude decreased with the increasing NiZnFe fractions; it decreased from 12.46 in the x = 1.0 product to 8.79 μB in the x = 3.0 NC product. The observed tendency in the variations of magneton numbers was in line with the observed tendency of Ms and Mr values with respect to the NiZnFe content.
The squareness ratios (SQR) = Mr/Ms were calculated (Table 2). An SQR can give information about the magnetic domains of a nanoparticle system. A theoretically predicted value above 0.50 is accredited to a single-domain structure [46]. However, an SQR < 0.5 is assigned to a multi-domain nature. In the present study, the SQR decreased from 0.403 to 0.214 at 300 K and from 0.424 to 0.298 at 10 K with the increase of the NiZnFe fraction in the produced products. All these values were below 0.5, which suggests a multi-magnetic domain nature for all products at both 300 and 10 K.
To further evaluate the effect of exchange-coupling within the produced products, the curves of the derivative of magnetization per applied magnetic field (dM/dH) against field were investigated (Figure 9) [52,53]. Typically, there will be a singular peak once the exchange coupling between the two phases is achieved. Nevertheless, binary separate maxima occur if the exchange coupling is still not completed [54]. In our case, two dissimilar peaks were observed in diverse products, illuminating that the reversal magnetization was unachievable by one-stage. These two distinctive peaks in dM/dH curves suggested that the magnetic spins of the soft and hard phases were switching individually.

3.4. Microwave Properties

Using the co-axial method (transmission line), measurements of the magnetic permeability and electrical permittivity (frequency dispersions of their real and imaginary parts) of the SrBaSmFe/x(NiZnFe) hard/soft ferrite NCs with varying hard/soft phases ratio 1:x (0.0 ≤ x ≤ 3.0) were performed. Figure 10 shows the dependences of the real (Figure 10a) and imaginary (Figure 10b) parts of the permittivity as a function of the frequency of the all composites ratio. It is clear that the chemical content (concentration of the soft phase-x) significantly affected the value of permittivity.
The obtained dispersions for the SrBaSmFe/x(NiZnFe) hard/soft ferrite NCs were in good agreement with the frequency dependences obtained from the standard theory for microwave properties in composites [40]. From the obtained results, it was clear that sample No. 6 did not have standart behavior. Since the various prepared hard/soft ferrite NCs were composed of two materials (Sr0.5Ba0.5Sm0.02Fe11.98O4 hard and Ni0.8Zn0.2Fe2O4 soft phases), the dielectric constant of these materials at frequencies from 1 to 14 GHz was from 4 to 5, and the value of the real part of the electrical permittivity of the composites practically did not vary with increasing frequency.
Only at frequencies above 14 GHz did the dependencies take on different values in frequency. For the imaginary part of the permittivity, the dependences of the materials were different: the losses in Sr0.5Ba0.5Sm0.02Fe11.98O4 were higher, and, therefore, the nature of the change in values was such that with an increase in the number of spinel, the graph of the frequency dependence mixed down along the y-axis.
With dipole polarization, the losses in the dielectric were minimal; therefore, the imaginary part of the permittivity did not vary with increasing frequency; see Figure 10. A significant decrease in the imaginary permittivity and an increase of losses were because, at these frequencies, a transition began from dipole to electronic polarization. This was due to the orientation of electrons in the electric field.
Figure 11 shows the dependences of the real (Figure 11a) and imaginary (Figure 11b) parts of the permeability as a function of the frequency of the all composites ratio.
For the real part of magnetic permeability, the values for hexaferrite were smaller (dependence of 6 at the very bottom) than those of the spinel; therefore, with an increase for spinel, the dependence graph mixed up along the y-axis. Theoretically, if pure spinel was measured, the dependences for composites can be predicted.

4. Conclusions

Functional hard/soft ferrite NCs (with the chemical formula of Sr0.5Ba0.5Sm0.02Fe11.98O4/x(Ni0.8Zn0.2Fe2O4)) (0.0 ≤ x ≤ 3.0) were fabricated by the one-pot citrate combustion method. According to the XRD results, all samples only contained initial SrBaSmFe and NiZnFe components in different ratios. The microstructure of the composite samples correlated with the shape and size of the initial components and their ratios. The morphology of hard, soft, and hard/soft NCs revealed three categories of particle shapes such as hexagonal plate, spherical, and an assembly of both hexagonal and spherical. M(H) hysteresis loops showed the hard ferrimagnetic nature of various produced products at both 300 and 10 K. The hard FM behavior of SrBaSmFe was considerably altered by raising the fraction of soft NiZnFe in the mixtures. The magnetization values (Ms, Mr, and Hc) were the highest for the SrBaSmFe/1.0(NiZnFe) hard/soft ferrite product (i.e., x = 1.0) and continuously reduced when raising the weight fraction of the NiZnFe soft phase. Microwave properties such as the frequency dispersions of the magnetic permeability and electrical permittivity (their real and imaginary parts) were measured with the co-axial method in the 1–18 GHz range. At these frequencies, the main mechanism contributing to the dielectric constant was dipole polarization. In the dipole polarization model, the process of orientation of the dipoles may not have time to induce changes in the external field; due to this, with increasing frequency, the real electrical permittivity decreased with increasing frequency. The real and imaginary magnetic permeabilities let us conclude that the behavior is typical for ferrimagnetics This means that the main losses in this type of composites can be attributed to electrical losses (dipole polarization).

Author Contributions

Conceptualization, M.A.A., Y.S., and A.V.T.; methodology, M.A.A., Y.S., and A.B.; data curation, S.V.T., M.G.V., and A.S.; formal analysis, D.S.K.; investigation, Y.S., M.A.A., N.A.A., M.A.G., A.V.T. and A.M.; microscopy observations, A.S.H.; writing—original draft, Y.S., M.A.A., A.B., and A.V.T.; writing—review and editing, Y.S., M.A.A., and A.V.T.; supervision, M.A.A., Y.S., and A.B. All authors have read and agreed to the published version of the manuscript.

Funding

This work was financially supported by the Deanship for Scientific Research (Project application No. 2020-164-IRMC) of Imam Abdulrahman Bin Faisal University (IAU—Saudi Arabia). The work was partially supported by the Russian Science Foundation (Agreement No. 19-72-10071 from 06 August 2019).

Acknowledgments

The authors are thankful to the Institute for Research and Medical Consultations (IMRC) of Imam Abdulrahman Bin Faisal University (IAU—Saudi Arabia) for providing lab facilities.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Kozlovskiy, A.L.; Zdorovets, M.V. The study of the structural characteristics and catalytic activity of Co/CoCo2O4 nanowires. Compos. Part B Eng. 2020, 191, 107968. [Google Scholar] [CrossRef]
  2. Kozlovskiy, A.L.; Kenzhina, I.E.; Zdorovets, M.V. FeCo–Fe2CoO4/Co3O4 nanocomposites: Phase transformations as a result of thermal annealing and practical application in catalysis. Ceram. Int. 2020, 46, 10262–10269. [Google Scholar] [CrossRef]
  3. Dukenbayev, K.; Korolkov, I.V.; Tishkevich, D.I.; Kozlovskiy, A.L.; Trukhanov, S.V.; Gorin, Y.G.; Shumskaya, E.E.; Kaniukov, E.Y.; Vinnik, D.A.; Zdorovets, M.V.; et al. Fe3O4 Nanoparticles for Complex Targeted Delivery and Boron Neutron Capture Therapy. Nanomaterials 2019, 9, 494. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  4. Pathania, A.; Thakur, P.; Trukhanov, A.V.; Trukhanov, S.V.; Panina, L.V.; Lüders, U.; Thakur, A.; Tomar, M.; Gupta, V. Development of tungsten doped Ni-Zn nano-ferrites with fast response and recovery time for hydrogen gas sensing application. Results Phys. 2019, 15, 102531. [Google Scholar] [CrossRef]
  5. Venturini, J.; Tonelli, A.M.; Wermuth, T.B.; Zampiva, R.Y.S.; Arcaro, S.; Da Cas Viegas, A.; Bergmann, C.P. Excess of cations in the sol-gel synthesis of cobalt ferrite (CoFe2O4): A pathway to switching the inversion degree of spinels. J. Magn. Magn. Mater. 2019, 482, 1–8. [Google Scholar] [CrossRef]
  6. Meng, X.F.; Hana, Q.X.; Sun, Y.J.; Liu, Y.F. Synthesis and microwave absorption properties of Ni0.5Zn0.5Fe2O4/BaFe12O19@polyaniline composite. Ceram. Int. 2019, 45, 2504–2508. [Google Scholar] [CrossRef]
  7. Almessiere, M.A.; Trukhanov, A.V.; Slimani, Y.; You, K.Y.; Trukhanov, S.V.; Trukhanova, E.L.; Esa, F.; Sadaqat, A.; Chaudhary, K.; Zdorovets, M.; et al. Correlation between composition and electrodynamics properties in nanocomposites based on hard/soft ferrimagnetics with strong exchange coupling. Nanomaterials 2019, 9, 202. [Google Scholar] [CrossRef] [Green Version]
  8. Xu, Y.F.; Man, Y.Q.; Xu, S.T.; Zan, F.L.; Zheng, G.H.; Dai, Z.X. Obtainment of exchange coupling coefficient of Ni0.6Zn0.4Fe2O4/SrFe12O19 composites. Mater. Lett. 2014, 131, 203–205. [Google Scholar] [CrossRef]
  9. Kneller, E.F.; Hawig, R. The exchange-spring magnet: A new material principle for permanent magnets. IEEE Trans. Magn. 1991, 27, 3560–3588. [Google Scholar] [CrossRef]
  10. Dong, J.; Zhang, Y.; Zhang, X.L.; Liu, Q.F.; Wang, J.B. Improved magnetic properties of SrFe12O19/FeCo core–shell nanofibers by hard/soft magnetic exchange–coupling effect. Mater. Lett. 2014, 120, 9–12. [Google Scholar] [CrossRef]
  11. Song, F.Z.; Shen, X.Q.; Liu, M.Q.; Xiang, J. Magnetic hard/soft nanocomposite ferrite aligned hollow microfibers and remanence enhancement. J. Colloid. Interface Sci. 2011, 354, 413–416. [Google Scholar] [CrossRef] [PubMed]
  12. Yang, H.B.; Lin, M.Y.; Dong, G.Q.; Hu, L.Y.; Zhang, Y.; Tan, J.Y. Enhanced remanence and (BH)max of BaFe12O19/CoFe2O4 composite ceramics prepared by the microwave sintering method. Mater. Chem. Phys. 2015, 160, 5–11. [Google Scholar] [CrossRef]
  13. Yang, H.B.; Liu, M.; Lin, Y.; Yang, Y.Y. Controlled growth of epitaxial wurtzite BeMgZnO alloy films and two microscopic origins of Be–Mg mutual stabilizing mechanism. J. Alloys Compd. 2015, 631, 335–339. [Google Scholar] [CrossRef]
  14. Kwon, H.W.; Jeong, I.C.; Kim, A.S.; Kim, D.H.; Namkung, S.; Jang, T.S.; Lee, D.H. Restoration of coercivity in crushed Nd–Fe–B magnetic powder. J. Magn. Magn. Mater. 2006, 304, e219–e221. [Google Scholar] [CrossRef]
  15. Liu, J.P.; Liu, Y.; Skomaski, R.; Sellmyer, D.J. Magnetic hardening in SmCox–Co multilayers and nanocomposites. J. Appl. Phys. 1999, 85, 4812–4814. [Google Scholar] [CrossRef]
  16. Goll, D.; Seeger, M.; Kronmuller, H. Magnetic and microstructural properties of nano crystalline exchange coupled PrFeB permanent magnets. J. Magn. Magn. Mater. 1998, 185, 49–60. [Google Scholar] [CrossRef]
  17. Jiang, J.S.; Pearson, J.E.; Liu, Z.Y.; Kabius, B.; Trasobares, S.; Miller, D.J.; Bader, S.D.; Lee, D.R.; Haskel, D.; Srajer, G.; et al. A new approach for improving exchange-spring magnets. J. Appl. Phys. 2005, 97, 10K311. [Google Scholar] [CrossRef] [Green Version]
  18. Xia, J.Y.; Ning, Y.; Luo, Y.H.; Chen, W.; Wu, X.H.; Wu, W.W.; Li, Q.Z.; Li, K.T. Structural and magnetic properties of soft/hard NiFe2O4@SrCo0.2Fe11.8O19 core/shell composite prepared by the ball-milling-assisted ceramic process. J. Mater. Sci. Mater. Electron. 2018, 29, 13903–13913. [Google Scholar] [CrossRef]
  19. Xia, J.Y.; Shen, Y.L.; Xiao, C.Y.; Chen, W.; Wu, X.H.; Wu, W.W.; Wang, Q.S.; Li, J.T. Structural and Magnetic Properties of Soft/Hard Mn0.6Zn0.4Fe2O4@Sr0.85Ba0.15Fe12O19 Core/Shell Composite Synthesized by the Ball-Milling-Assisted Ceramic Proces. J. Electron. Mater. 2018, 47, 6811–6820. [Google Scholar] [CrossRef]
  20. Trukhanov, A.V.; Algarou, N.A.; Slimani, Y.; Almessiere, M.A.; Baykal, A.; Tishkevich, D.I.; Vinnik, D.A.; Vakhitov, M.G.; Klygach, D.S.; Silibin, M.V.; et al. Peculiarities of the microwave properties of hard-soft functional composites SrTb0.01Tm0.01Fe11.98O19-AFe2O4 (A = Co, Ni, Zn, Cu and Mn). RSC Adv. 2020, 10, 32638–32651. [Google Scholar] [CrossRef]
  21. Harikrishnan, V.; Vizhi, R.E. A study on the extent of exchange coupling between (Ba0.5Sr0.5Fe12O19)1−x(CoFe2O4)x magnetic nanocomposites synthesized by solgel combustion method. J. Magn. Magn. Mater. 2016, 418, 217–223. [Google Scholar] [CrossRef]
  22. Radmanesh, M.; Ebrahimi, S.S. Synthesis and magnetic properties of hard/soft SrFe12O19/Ni0.7Zn0.3Fe2O4 nanocomposite magnets. J. Magn. Magn. Mater. 2012, 324, 3094–3098. [Google Scholar] [CrossRef]
  23. Chen, W.; Xiao, C.Y.; Huang, C.; Wu, X.H.; Wu, W.W.; Wang, Q.S.; Li, J.T.; Zhou, K.W.; Huang, Y.F. Exchange-coupling behavior in soft/hard Li0.3Co0.5Zn0.2Fe2O4/SrFe12O19 core/shell composite synthesized by the two-step ball-milling-assisted ceramic process. Mater. Sci. Mater. Electron. 2019, 30, 1579–1590. [Google Scholar] [CrossRef]
  24. Feng, W.; Liu, H.; Hui, P.; Yang, H.; Li, J.; Wang, J.S. Preparation and Properties of SrFe12O19/ZnFe2O4 Core/Shell Nano-powder Microwave Absorber. Integr. Ferroelectr. 2014, 152, 120–126. [Google Scholar] [CrossRef]
  25. Li, D.; Wang, F.; Xia, A. A facile way to realize exchange-coupling interaction in hard/soft magnetic composites. J. Magn. Magn. Mater. 2016, 41, 355–358. [Google Scholar] [CrossRef]
  26. Meng, X.F.; Zhu, Y.J.; Xu, S.; Liu, T. Facile synthesis of shell–core polyaniline/SrFe12O19 composites and magnetic properties. RSC Adv. 2016, 6, 4946–4949. [Google Scholar] [CrossRef]
  27. Bader, S. Colloquium: Opportunities in nano magnetism. Rev. Mod. Phys. 2006, 78, 1. [Google Scholar] [CrossRef]
  28. Algarou, N.A.; Slimani, Y.; Almessiere, M.A.; Alahmari, F.S.; Vakhitov, M.G.; Klygach, D.S.; Trukhanov, S.V.; Trukhanov, A.V.; Baykal, A. Magnetic and microwave properties of SrFe12O19/MCe0.04Fe1.96O4 (M =Cu, Ni, Mn, Co and Zn) hard/soft nanocomposites. J. Mat. Res. Tech. 2020, 9, 5858–5870. [Google Scholar] [CrossRef]
  29. Algarou, N.A.; Slimani, Y.; Almessiere, M.A.; Rehman, S.; Younas, M.; Unal, B.; Demir Korkmaz, A.; Gondal, M.A.; Trukhanov, A.V.; Baykal, A.; et al. Developing the magnetic, dielectric and anticandidal characteristics of SrFe12O19/(Mg0.5Cd0.5Dy0.03Fe1.97O4)x hard/soft ferrite nanocomposites. J. Taiwan Inst. Chem. Eng. 2020, 113, 344–362. [Google Scholar] [CrossRef]
  30. Lewis, L.H.; Jiménez-Villacorta, F. Perspectives on permanent magnetic materials for energy conversion and power generation. Metall. Mater. Trans. A 2013, 44, 2–20. [Google Scholar] [CrossRef]
  31. Hazra, S.; Ghosh, N. Preparation of nano ferrites and their applications. J. Nanosci. Nanotechnol. 2014, 14, 1983–2000. [Google Scholar] [CrossRef]
  32. Pardavi-Horvath, M. Microwave applications of soft ferrites. J. Magn. Magn. Mater. 2000, 215, 171–183. [Google Scholar] [CrossRef]
  33. Harris, V.G. Modern microwave ferrites. IEEE Trans. Magn. 2012, 48, 31075–31104. [Google Scholar] [CrossRef]
  34. Mehdipour, M.; Sholrollahi, H. Comparison of microwave absorption properties of SrFe12O19, SrFe12O19/NiFe2O4 and NiFe2O4 particles. J. Appl. Phys. 2013, 113, 043906. [Google Scholar] [CrossRef]
  35. Hilczer, A.; Kowalska, K.; Markiewicz, E.; Adam, P. Dielectric and magnetic response of SrFe12O19-CoFe2O4 composites obtained by solid state reaction. Mater. Sci. Eng. 2016, 207, 47–55. [Google Scholar] [CrossRef]
  36. Meng, X.F.; Hana, Q.X.; Sun, Y.J.; Liu, Y.F. Enhancements of saturation magnetization and coercivity in Ni0.5Zn0.5Fe2O4/SrFe12O19 composite powders by exchange-coupling mechanism. Ceram. Int. 2019, 45, 2504–2508. [Google Scholar] [CrossRef]
  37. Han, Q.X.; Meng, X.F.; Lu, C.H. Exchange-coupled Ni0.5Zn0.5Fe2O4/SrFe12O19 composites with enhanced microwave absorption performance. J. Alloys Compd. 2018, 768, 742–749. [Google Scholar] [CrossRef]
  38. Saini, A.; Thakur, A.; Thakur, P. Effective permeability and miniaturization estimation of ferrite-loaded microstrip patch antenna. J. Electron. Mater. 2016, 45, 4162–4170. [Google Scholar] [CrossRef]
  39. Trukhanov, A.V.; Astapovich, K.A.; Turchenko, V.A.; Almessiere, M.A.; Slimani, Y.; Baykal, A.; Sombra, A.S.B.; Jotania, R.B.; Singh, C.; Zubar, T.I.; et al. Influence of the dysprosium ions on structure, magnetic characteristics and origin of the reflection losses in the Ni-Co spinels. J. Alloys Compd. 2020, 841, 155667. [Google Scholar] [CrossRef]
  40. Malkin, A.I.; Knyazev, N.C. Experimental set up for the measurements of dielectric permittivity and magnetic permeability in dielectric materials. In Proceedings of the XIV International Conference Physics and Technical Applications of Wave Processes, Samara, Russia, 24–26 November 2016; pp. 223–224. (In Russian). [Google Scholar]
  41. Torkian, S.; Ghasemi, A.; Razavi, R.S. Magnetic properties of hard-soft SrFe10Al2O19/Co0.8Ni0.2Fe2O4 ferrite synthesized by one-pot sol–gel auto-combustion. J. Magn. Magn. Mater. 2016, 416, 408–416. [Google Scholar] [CrossRef]
  42. Almessiere, M.A.; Slimani, Y.; Gungunes, H.; Manikandan, A.; Baykal, A. Investigation of the effects of Tm3+ on the structural, microstructural, optical, and magnetic properties of Sr hexaferrites. Results Phys. 2019, 13, 102166. [Google Scholar] [CrossRef]
  43. Almessiere, M.A.; Slimani, Y.; El Sayed, H.S.; Baykal, A. Morphology and magnetic traits of strontium nanohexaferrites: Effects of manganese/yttrium co-substitution. J. Rare Earths 2019, 37, 732–740. [Google Scholar] [CrossRef]
  44. Pahwa, C.; Narang, S.B.; Sharma, P. Composition dependent magnetic and microwave properties of exchange-coupled hard/soft nanocomposite ferrite. J. Alloys Compd. 2020, 815, 152391. [Google Scholar] [CrossRef]
  45. Torkian, S.; Ghasemi, A. Energy product enhancement in sufficiently exchange-coupled nanocomposite ferrites. J. Magn. Magn. Mater. 2019, 469, 119–127. [Google Scholar] [CrossRef]
  46. Stoner, E.C.; Wohlfarth, E.P. A Mechanism of Magnetic Hysteresis in Heterogeneous Alloys. Philos. Trans. R. Soc. Lond. Ser. A Math. Phys. Sci. 1948, 240, 599–642. [Google Scholar] [CrossRef]
  47. Almessiere, M.A.; Slimani, Y.; Baykal, A. Impact of Nd-Zn co-substitution on microstructure and magnetic properties of SrFe12O19 nanohexaferrite. Ceram. Int. 2019, 45, 963–969. [Google Scholar] [CrossRef]
  48. Almessiere, M.A.; Slimani, Y.; El Sayed, H.S.; Baykal, A.; Ercan, I. Microstructural and magnetic investigation of vanadium-substituted Sr-nanohexaferrite. J. Magn. Magn. Mater. 2019, 471, 124–132. [Google Scholar] [CrossRef]
  49. Algarou, N.A.; Slimani, Y.; Almessiere, M.A.; Baykal, A.; Guner, S.; Manikandan, A.; Ercan, I. Enhancement on the exchange coupling behavior of SrCo0.02Zr0.02Fe11.96O19/MFe2O4 (M = Co, Ni, Cu, Mn and Zn) as hard/soft magnetic nanocomposites. J. Magn. Magn. Mater. 2020, 499, 166308. [Google Scholar] [CrossRef]
  50. Algarou, N.A.; Slimani, Y.; Almessiere, M.A.; Güner, S.; Baykal, A.; Ercan, I.; Kögerler, P. Exchange-coupling effect in hard/soft SrTb0.01Tm0.01Fe11.98O19/AFe2O4 (where A = Co, Ni, Zn, Cu and Mn) composites. Ceram. Int. 2020, 46, 7089–7098. [Google Scholar] [CrossRef]
  51. Almessiere, M.A.; Demir Korkmaz, A.; Slimani, Y.; Nawaz, M.; Ali, S.; Baykal, A. Magneto-optical properties of rare earth metals substituted Co-Zn spinel nanoferrites. Ceram. Int. 2019, 45, 3449–3458. [Google Scholar] [CrossRef]
  52. Almessiere, M.A.; Slimani, Y.; Baykal, A. Exchange spring magnetic behavior of Sr0.3Ba0.4Pb0.3Fe12O19/(CuFe2O4)x nanocomposites fabricated by a one-pot citrate sol-gel combustion method. J. Alloys Compd. 2018, 762, 389–397. [Google Scholar] [CrossRef]
  53. Almessiere, M.A.; Slimani, Y.; Baykal, A. Structural, morphological and magnetic properties of hard/soft SrFe12−xVxO19/(Ni0.5Mn0.5Fe2O4)y nanocomposites: Effect of vanadium substitution. J. Alloys Compd. 2018, 767, 966–975. [Google Scholar] [CrossRef]
  54. Algarou, N.A.; Slimani, Y.; Almessiere, M.A.; Baykal, A. Exchange-coupling behavior in SrTb0.01Tm0.01Fe11.98O19/(CoFe2O4)x hard/soft nanocomposites. New. J. Chem. 2020, 44, 5800–5808. [Google Scholar] [CrossRef]
Figure 1. Synthesis stages of SrBaSmFe/x(NiZnFe) (0.0 ≤ x ≤ 3.0) nanocomposites (NCs).
Figure 1. Synthesis stages of SrBaSmFe/x(NiZnFe) (0.0 ≤ x ≤ 3.0) nanocomposites (NCs).
Nanomaterials 10 02134 g001
Figure 2. XRD powder patterns of (a) pure SrBaSmFe, NiZnFe, and (b) SrBaSmFe/(NiZnFe)x hard/soft ferrite nanocomposites (1 ≤ x ≤ 3).
Figure 2. XRD powder patterns of (a) pure SrBaSmFe, NiZnFe, and (b) SrBaSmFe/(NiZnFe)x hard/soft ferrite nanocomposites (1 ≤ x ≤ 3).
Nanomaterials 10 02134 g002aNanomaterials 10 02134 g002b
Figure 3. FE-SEM images of pure SrBaSmFe, pure NiZnFe, SrBaSmFe/(NiZnFe)1.5 NC, and SrBaSmFe/(NiZnFe)2.5 NC.
Figure 3. FE-SEM images of pure SrBaSmFe, pure NiZnFe, SrBaSmFe/(NiZnFe)1.5 NC, and SrBaSmFe/(NiZnFe)2.5 NC.
Nanomaterials 10 02134 g003
Figure 4. Energy-dispersive X-ray (EDX) and elemental mapping of hard/soft ferrite SrBaSmFe/(NiZnFe)x NCs with x = 1.5 and 2.5.
Figure 4. Energy-dispersive X-ray (EDX) and elemental mapping of hard/soft ferrite SrBaSmFe/(NiZnFe)x NCs with x = 1.5 and 2.5.
Nanomaterials 10 02134 g004
Figure 5. TEM (left) and HR-TEM (right) images of hard/soft ferrite SrBaSmFe/(NiZnFe)x NCs with x = 1.5 and 2.5.
Figure 5. TEM (left) and HR-TEM (right) images of hard/soft ferrite SrBaSmFe/(NiZnFe)x NCs with x = 1.5 and 2.5.
Nanomaterials 10 02134 g005
Figure 6. M(H) hysteresis curves recorded at (a,b) T = 300 K and (c,d) T = 10 K for Ni0.8Zn0.2Fe2O4 (NiZnFe) and Sr0.5Ba0.5Sm0.04Fe11.96O19 (SrBaSmFe) samples. (b) and (d) are enlarged views of magnetic hysteresis loops.
Figure 6. M(H) hysteresis curves recorded at (a,b) T = 300 K and (c,d) T = 10 K for Ni0.8Zn0.2Fe2O4 (NiZnFe) and Sr0.5Ba0.5Sm0.04Fe11.96O19 (SrBaSmFe) samples. (b) and (d) are enlarged views of magnetic hysteresis loops.
Nanomaterials 10 02134 g006
Figure 7. M(H) hysteresis curves performed at (a,b) T = 300 K and (c,d) T = 10 K for hard/soft ferrite SrBaSmFe/(NiZnFe)x NCs (1.0 ≤ x ≤ 3.0) products.
Figure 7. M(H) hysteresis curves performed at (a,b) T = 300 K and (c,d) T = 10 K for hard/soft ferrite SrBaSmFe/(NiZnFe)x NCs (1.0 ≤ x ≤ 3.0) products.
Nanomaterials 10 02134 g007
Figure 8. Variations in (a) saturation magnetization (Ms), (b) remnant magnetization (Mr), and (c) coercivity (Hc) at both 300 and 10 K for various produced hard/soft ferrite SrBaSmFe/(NiZnFe)x NCs (1.0 ≤ x ≤ 3.0) products.
Figure 8. Variations in (a) saturation magnetization (Ms), (b) remnant magnetization (Mr), and (c) coercivity (Hc) at both 300 and 10 K for various produced hard/soft ferrite SrBaSmFe/(NiZnFe)x NCs (1.0 ≤ x ≤ 3.0) products.
Nanomaterials 10 02134 g008
Figure 9. dM/dH vs. H plots performed at (a) T = 300 K and (b) T = 10 K for various prepared hard/soft ferrite SrBaSmFe/(NiZnFe)x NCs (0 ≤ x ≤ 3) products.
Figure 9. dM/dH vs. H plots performed at (a) T = 300 K and (b) T = 10 K for various prepared hard/soft ferrite SrBaSmFe/(NiZnFe)x NCs (0 ≤ x ≤ 3) products.
Nanomaterials 10 02134 g009
Figure 10. Frequency dispersions of the real part (a) and imaginary part (b) of permittivity for the SrBaSmFe/(NiZnFe)x NCs.
Figure 10. Frequency dispersions of the real part (a) and imaginary part (b) of permittivity for the SrBaSmFe/(NiZnFe)x NCs.
Nanomaterials 10 02134 g010
Figure 11. Frequency dispersions of the real part (a) and imaginary part (b) of permeability for the SrBaSmFe/(NiZnFe)x NCs.
Figure 11. Frequency dispersions of the real part (a) and imaginary part (b) of permeability for the SrBaSmFe/(NiZnFe)x NCs.
Nanomaterials 10 02134 g011
Table 1. Crystallites size (DXRD), lattice parameters, and phase fractions calculated for both hard (107 plane) and soft (311 plane) phases in hard/soft ferrite nanocomposites of SrBaSmFe/(NiZnFe)x (0 ≤ x ≤ 3).
Table 1. Crystallites size (DXRD), lattice parameters, and phase fractions calculated for both hard (107 plane) and soft (311 plane) phases in hard/soft ferrite nanocomposites of SrBaSmFe/(NiZnFe)x (0 ≤ x ≤ 3).
NanocompositeDXRD (nm)Hard PhaseSoft Phase
SoftHarda = b (Å)c (Å)Fraction (%)a = b = c (Å)Fraction (%)
SrBaSmFe-50.95.884523.1037100--
SrBaSmFe/(NiZnFe)1.021.548.35.886823.096381.18.359118.9
SrBaSmFe/(NiZnFe)1.526.137.85.887823.117764.28.358135.8
SrBaSmFe/(NiZnFe)2.027.755.75.894823.115253.38.353646.7
SrBaSmFe/(NiZnFe)2.530.449.95.895023.134246.28.352153.8
SrBaSmFe/(NiZnFe)3.050.382.95.900223.051229.08.343971.0
NiZnFe44.1----8.3553100
Table 2. Squareness ratio (SQR) and magneton numbers (nB) of the hard/soft ferrite products of SrBaSmFe/(NiZnFe)x NCs where x = 1.0 up to 3.0.
Table 2. Squareness ratio (SQR) and magneton numbers (nB) of the hard/soft ferrite products of SrBaSmFe/(NiZnFe)x NCs where x = 1.0 up to 3.0.
H:S RatioSQRnB (μB)
300 K10 K300 K10 K
1:1.00.4030.4248.1412.46
1:1.50.3450.3827.1510.99
1:2.00.3170.3526.5010.01
1:2.50.2780.3246.039.31
1:3.00.2140.2985.688.79
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Algarou, N.A.; Slimani, Y.; Almessiere, M.A.; Sadaqat, A.; Trukhanov, A.V.; Gondal, M.A.; Hakeem, A.S.; Trukhanov, S.V.; Vakhitov, M.G.; Klygach, D.S.; et al. Functional Sr0.5Ba0.5Sm0.02Fe11.98O4/x(Ni0.8Zn0.2Fe2O4) Hard–Soft Ferrite Nanocomposites: Structure, Magnetic and Microwave Properties. Nanomaterials 2020, 10, 2134. https://doi.org/10.3390/nano10112134

AMA Style

Algarou NA, Slimani Y, Almessiere MA, Sadaqat A, Trukhanov AV, Gondal MA, Hakeem AS, Trukhanov SV, Vakhitov MG, Klygach DS, et al. Functional Sr0.5Ba0.5Sm0.02Fe11.98O4/x(Ni0.8Zn0.2Fe2O4) Hard–Soft Ferrite Nanocomposites: Structure, Magnetic and Microwave Properties. Nanomaterials. 2020; 10(11):2134. https://doi.org/10.3390/nano10112134

Chicago/Turabian Style

Algarou, Norah A., Yassine Slimani, Munirah A. Almessiere, Ali Sadaqat, Alex V. Trukhanov, Mohammad A. Gondal, Abbas S. Hakeem, Sergei V. Trukhanov, Maksim G. Vakhitov, Denis S. Klygach, and et al. 2020. "Functional Sr0.5Ba0.5Sm0.02Fe11.98O4/x(Ni0.8Zn0.2Fe2O4) Hard–Soft Ferrite Nanocomposites: Structure, Magnetic and Microwave Properties" Nanomaterials 10, no. 11: 2134. https://doi.org/10.3390/nano10112134

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.